Properties Relevant to Coloring and Additives
PE is a semi-crystalline polymer. Its melting temperature (Tm) is 110–135 °C, its glass transition temperature (Tg) is −110 °C and its density is 0.92–0.96 g/cm³. Typical melt temperature is 180–240 °C for LDPE and 210–270 °C for HDPE; mold temperature is 20–60 °C for both.
- Migration: Pigment migration risk is low in polyolefins (PE/PP); grade 4–5 on the gray scale.
- Thermal degradation: Under high temperature and shear, PE undergoes crosslinking, which shows up as gels and black specks in film.
- Film surface: Smooth PE film layers tend to stick to each other (blocking) when wound, and the friction coefficient of unadditivated film is high. For this reason, slip and antiblock are frequently used in film recipes.
- UV degradation: In outdoor PE products, UV radiation causes color loss, cracking and chalking.
Recommended Colorex Masterbatches and Additives
- Color masterbatch: Produced with a compatible carrier for LDPE, LLDPE and HDPE; used at 2.0–4.0% in thin film and fiber and 1.5–3.0% in injection, blow molding and pipe.
- White masterbatch: 2.5–6.0% is recommended in thin film and IML and 1.5–4.0% in standard injection, blow molding and profile; series loaded with 60–70% rutile TiO₂ are available for ultra-thin films.
- Black masterbatch: Used at 5.0–6.5% (2.5–5.5% for 40–50% loaded series) in PE100 pipe and UV-protected outdoor products to provide UV protection and opacity.
- Slip masterbatch: Erucamide or oleamide based products reduce the dynamic coefficient of friction from 0.60–0.80 to below the 0.15–0.20 band; dosage 1.0–3.0%.
- Antiblock masterbatch: Prevents layers from sticking by creating micro peaks of 2–6 μm on the film surface; 1.0–3.0% in general film and 1.0–2.0% with synthetic silica in thin transparent film.
- Processing aid (PPA): Reduces sharkskin and die build-up in LLDPE, mLLDPE and HDPE; 0.5–2.0% in continuous production and 2.0–3.0% during the first 30–60 minutes.
- UV & light stabilizer: Protects greenhouse covers, mulch film and outdoor products; 2.0–6.0% in thin film and greenhouse covers.
- Filler masterbatch: Used at 5.0–20.0% in bag and film extrusion to balance cost and stiffness.
Notes by Process
- Blown and cast film: The typical color masterbatch dosage in thin and blown film is 1–3%. Since agglomerated pigment leads to pinholes and screen clogging, a product with a low FPV should be selected.
- Pressure pipe (PE100): A carbon black content of 2.0–2.5% in the final product is targeted. Dispersion is expected to be grade 3 or below according to ISO 18553.
- Blow molding (bottles, canisters): The typical color masterbatch dosage is 2–5%; opacity and gloss are targeted together. In HDPE blow-molded products, filler masterbatch can be used at 5–20%.
- Injection (crates, buckets): Antistatic masterbatch is used in buckets and containers that should not collect dust on the shelf; dosage for migratory series is 1.0–3.0%.
Points to Watch
- The carrier resin should be selected according to the melt flow (MFI) of the film, pipe or injection grade.
- Pigments and fillers can affect the migration of slip to the surface; in recipes that combine color and slip, the friction coefficient should be measured and verified in the laboratory.
- Mineral-containing additives such as antiblock and TiO₂ can slow PPA's coating of the die surface; in these combinations, the PPA ratio is determined by project-specific testing.
- Acidic pigments and additives and halogenated flame retardant systems can neutralize HALS; the appropriate HALS type should be selected in UV-protected recipes.
Frequently Asked Questions
At what ratio is black masterbatch used in PE100 pipes?
In PE100 water and natural gas pipes, a carbon black content of 2.0–2.5% in the final product is targeted. This is achieved with a dosage of 5.0–6.5% in standard series and 2.5–5.5% in series loaded with 40–50% carbon black.
How are blocking and high friction prevented in PE film?
Layer sticking is prevented with antiblock masterbatch and high friction with slip masterbatch. The two additives can be combined in a single granule; the friction coefficient of the combined recipe is measured and verified in the laboratory.
Why does sharkskin appear on LLDPE film?
LLDPE and mLLDPE with a narrow molecular weight distribution exceed the critical shear stress when passing through the die at high speed, creating surface roughness. Processing aid (PPA) masterbatch forms a slip layer on the die metal and reduces this roughness and die build-up.