Color

Production color differs from the laboratory approval

Likely cause
The temperature/shear difference between the laboratory and mass production changes the ΔE.
Solution
Color approval must be done under actual process conditions; process simulation is essential.
Related product
Color Masterbatch
Color

Color varies from batch to batch with regrind or PCR raw material

Likely cause
The base color of recycled raw material can vary from batch to batch.
Solution
Use a high-opacity color masterbatch that covers the base color; dosage is generally 2.5–4.0%. Working with your own regrind sample gives the most accurate result.
Related product
Color Masterbatch
Color

Parts that match under store lighting look different in daylight

Likely cause
Parts matched with different pigment combinations can look the same under TL84 store lighting but shift to different shades in D65 daylight (metamerism).
Solution
The color formula is designed to avoid metamerism under D65, TL84 and A light sources and is checked in a multi-light booth.
Related product
Color Masterbatch
Color

White parts turn yellow from heat

Likely cause
Thermo-oxidative degradation caused by heat.
Solution
An antioxidant-additive, heat-stable masterbatch stabilizes the melt and keeps the white long-lasting.
Related product
Antioxidant Masterbatch
Color

White outdoor products turn yellow in the sun

Likely cause
The sun's UV rays break down polymer chains (photo-oxidation).
Solution
Use an outdoor white masterbatch with surface-treated rutile TiO₂ of low photocatalytic activity, together with antioxidants that do not cause phenolic yellowing and a suitable dosage of HALS UV stabilizer.
Related product
White Masterbatch
Color

Red, yellow, orange and purple outdoor products fade quickly in the sun

Likely cause
Vivid shades mostly require organic pigments, and economical organic pigments fade quickly under UV.
Solution
Use a color masterbatch formulated with high-performance, outdoor-grade organic/inorganic hybrid pigments.
Related product
Color Masterbatch
Color

Artificial grass fibers fade in the sun

Likely cause
The lightfastness of the colorant is insufficient.
Solution
Use a masterbatch rated 7–8 on the Blue Wool Scale and containing UV stabilizer.
Related product
UV & Light Stabilizer
Color

Gray blotches appear in white injection-molded parts

Likely cause
Contamination or poor dispersion.
Solution
Resolved with a clean process and a high-purity white masterbatch.
Related product
White Masterbatch
Color

Color transfers from food film to the food (bleeding)

Likely cause
When a pigment exceeds its solubility limit in the polymer, it blooms to the surface or moves into an adjacent phase (bleeding).
Solution
Use high-molecular-weight, low-migration pigments (e.g. PY151) to prevent color transfer to the food.
Related product
Yellow Pigment
Color

Color streaks (striping) in sack yarn

Likely cause
Dosage irregularity.
Solution
Gravimetric dosing and a high-color-strength masterbatch give a homogeneous color.
Related product
Color Masterbatch
Surface

Deposits build up on the mold, rollers or machine surfaces (plate-out)

Likely cause
The migration tendency of additives, overdosing (e.g. slip or antistatic) or an incompatible formulation makes additives deposit on metal surfaces.
Solution
Choose the right additive, a suitable dosage and good dispersion; use a compatible, low-migration series.
Related product
Slip Masterbatch
Surface

Silver streaks appear on injection-molded parts

Likely cause
Most commonly, the raw material or recycled polymer was not dried sufficiently and the moisture left in the melt evaporates; thermal degradation can also contribute.
Solution
Dry the masterbatch and polymer and optimize the process temperature; where moisture is the cause, CaO-containing desiccant masterbatch chemically binds the water.
Related product
Desiccant & Antigas Masterbatch
Surface

Bubbles and pores form on the product surface

Likely cause
Moisture in the raw material evaporates in the melt.
Solution
Dry the polymer at 80 °C or use CaO-containing desiccant masterbatch; together with proper drying, bubbles are largely prevented.
Related product
Desiccant & Antigas Masterbatch
Surface

Sink marks on thick-walled parts

Likely cause
Thick sections shrink inward as they cool.
Solution
Add 0.5–1.0% endothermic foaming masterbatch to the formulation; in thick-walled armrests and pallets, sink marks disappear completely at 0.8%.
Related product
Foaming Masterbatch
Surface

The part surface scratches easily and the scratch looks white

Likely cause
A hard object creates micro-cracks on the surface; in talc-filled PP, talc particles separate from the matrix and leave a white mark.
Solution
UHMW siloxane anti-scratch masterbatch lowers the coefficient of friction; at 1.5–2.5% it prevents white scratch marks from transport and use.
Related product
Anti-Scratch Masterbatch
Surface

A white mark remains when a black or dark part is bent (stress whitening)

Likely cause
Excessive bending forms microscopic voids in the polymer matrix, and these voids scatter light.
Solution
Fine-particle carbon black, high dispersion and an elastomer-compatible carrier markedly reduce this whitening.
Related product
Black Masterbatch
Surface

Black specks (charring) appear in the product

Likely cause
The residence time is exceeded or the heat is too high; burned polymer/pigment on the barrel wall, screw flights or nozzle tip breaks off into the product.
Solution
Lower the temperature by 15 °C and add a thermal stabilizer; regular use of a purging compound strips the carbon layers before they harden.
Related product
Machine and Screw Purging Compound
Surface

White specks appear in film or raffia tape

Likely cause
Contamination or poor dispersion.
Solution
Resolved with a high-purity, well-dispersed masterbatch.
Surface

The extruded surface comes out rough like sharkskin (melt fracture)

Likely cause
When line speed or the LLDPE/mLLDPE ratio increases, friction at the die lip creates a rough, dull surface.
Solution
Processing aid (PPA) masterbatch reduces the shear stress at the die lip to zero; with 1.0–1.5% PPA, sharkskin is completely eliminated and head pressure drops by 10–20%.
Related product
Processing Aid (PPA) Masterbatch
Film

Film layers stick together and bag mouths will not open (blocking)

Likely cause
Close contact between flat film surfaces, combined with winding tension or stacking load and heat, increases the attractive forces between them.
Solution
Antiblock masterbatch physically reduces the contact area; in 25 μm LDPE/LLDPE film, 1.5% synthetic silica-based antiblock lowers the blocking force from around 80 g to below 15 g.
Related product
Antiblock Masterbatch
Film

Film snags, does not slip or does not open on the packaging machine

Likely cause
The coefficient of friction (COF) is high; at too low a slip dosage, too little amide reaches the surface.
Solution
Slip masterbatch lowers the COF; on FFS lines, 1.5% erucamide-based slip stops the film sticking to the forming collar and raises machine speed by 15–25%.
Related product
Slip Masterbatch
Film

Pinholes form in thin film

Likely cause
TiO₂ agglomeration.
Solution
Use a high-dispersion, fine-particle white (titanium) masterbatch; white masterbatch loaded with 60–70% rutile TiO₂ gives thin films a light barrier without pinholes or screen clogging.
Related product
White Masterbatch
Film

The inside of packaging film fogs up and hides the product

Likely cause
Warm, humid air condenses on the cold film surface; because PE and PP have low surface energy, water forms small droplets that scatter light.
Solution
Use anti-fog masterbatch; cold-chain vegetable, fruit and meat packaging films use a dosage of 1.0–2.0%.
Related product
Anti-Fog Masterbatch
Film

Water drops form inside greenhouse film and drip onto plants

Likely cause
In greenhouse film without anti-fog, the drops reduce incoming light by 15–20%; dripping cold water causes plant diseases and the lens effect of the drops causes leaf burns.
Solution
In agricultural LDPE greenhouse covers, 2.0–3.0% anti-fog masterbatch prevents cold water from dripping onto plants and causing burn spots.
Related product
Anti-Fog Masterbatch
Film

Packaging film or bags tear during packing

Likely cause
The film's strength is low.
Solution
Use a well-dispersed masterbatch that preserves tensile strength, at the correct dosage; in heavy-duty sacks and regrind-containing PE/PP films, Anti-Split masterbatch increases MD/TD tear and puncture resistance.
Related product
Anti-Split Masterbatch
Processing

Color changeovers waste a lot of material and time

Likely cause
Cleaning the barrel with virgin resin takes long: a black-to-white change can mean 80–100 kg of resin loss and 2 hours of downtime.
Solution
Use a purging compound and temporarily raise the heat by 10 °C; with 1.5–2 barrel volumes, clean production is reached in 15–20 minutes with 60–75% less raw material loss.
Related product
Machine and Screw Purging Compound
Processing

An old color streak remains in pipe or profile

Likely cause
Old color accumulates in the dead zones behind the spider legs in the die.
Solution
While the purging compound passes through the die, lower and raise the extruder speed in 1–2 minute cycles; the pressure change strips the adhering pigments.
Related product
Machine and Screw Purging Compound
Processing

Parts are hard to demold and ejector marks remain

Likely cause
The part adheres to the mold wall; contaminants, degraded low-molecular-weight chains and high filler levels in regrind/PCR increase sticking.
Solution
Mold release masterbatch eliminates external sprays and prevents ejector marks; with 0.8% silicone-free mold release, cycle time is shortened by 8–12%.
Related product
Mold Release Masterbatch
Processing

The extruder screen or filter clogs

Likely cause
Coarse particles and impurities in the masterbatch cause pressure build-up at the screen.
Solution
Use a high-purity, low-FPV masterbatch; every Mono Masterbatch batch undergoes an FPV (Filter Pressure Value) test.
Related product
Mono Masterbatch (SPC)
Processing

Bubble bursts and tape breaks in regrind PE bag or calcite raffia production

Likely cause
Moisture in the polymer turns into steam at processing temperature and forms pressurized gas bubbles in the melt; in some polymers it also lowers mechanical strength through hydrolysis.
Solution
1.5–2.5% desiccant masterbatch stops moisture-induced bubble bursts, tape breaks and surface bubbles.
Related product
Desiccant & Antigas Masterbatch
Processing

PP/HDPE lids, buckets or crates warp

Likely cause
Some organic pigments act as nucleating agents in semi-crystalline polymers, so the part shrinks differently in the flow and transverse directions.
Solution
Use a low-warpage color masterbatch with pigment architectures of low nucleating effect; critical parts are checked with test plaques in the laboratory.
Related product
Color Masterbatch
Processing

Build-up forms at the die lip

Likely cause
Low-molecular-weight fractions, pigments and fillers separating from the melt collect at the die exit; deposits that break off cause streaks or spots.
Solution
Use processing aid (PPA) masterbatch together with clean-carrier masterbatches; PPA forms a slippery layer on the die surface and stops build-up.
Related product
Processing Aid (PPA) Masterbatch
Durability

The outdoor product surface turns matte and chalky

Likely cause
UV rays break down polymer chains; micro-cracks on the surface scatter light and expose pigment and filler particles.
Solution
Use a UV stabilizer with the right absorber–HALS balance; in Mediterranean conditions, a 2.0–3.0% HALS + UV package provides 3–5 years of outdoor durability.
Related product
UV & Light Stabilizer
Durability

PP crates break in cold storage

Likely cause
The glass transition temperature (Tg) of homopolymer PP is around 0 °C; below freezing it loses its flexibility and breaks like glass.
Solution
Use HDPE or high-impact block copolymer PP; with homopolymer or regrind, add a POE-based impact modifier with a low Tg. With 6% POE, drop and cold impact strength increase 3–5 times.
Related product
Impact Modifier & Compatibilizer
Durability

Parts made from mixed PP+PE regrind are brittle and the surface peels

Likely cause
PP and PE do not mix in the melt; on cooling, weak boundaries form between them and cracks travel along these boundaries.
Solution
PP+PE compatibilizer masterbatch lowers the tension between the two phases; 3% compatibilizer ends layer delamination and brittleness.
Related product
Impact Modifier & Compatibilizer
Durability

Parts become brittle and dull with high calcite or talc

Likely cause
A high calcite content lowers impact resistance and makes the color pastel and matte.
Solution
Use a high-pigment-loading color masterbatch together with a balanced impact modifier/compatibilizer and gloss-enhancing additives.
Related product
Impact Modifier & Compatibilizer
Durability

MFI jumps and the material yellows over regrind and recycling cycles

Likely cause
Each processing cycle consumes the existing antioxidant; chain scission raises the MFI.
Solution
Restabilize with antioxidant masterbatch; on lines running above 250 °C, 0.5–1.0% stops the MFI jump and the deterioration of the yellowness index (YI) even in the 3rd and 4th regrind cycles.
Related product
Antioxidant Masterbatch
Durability

PP raffia tapes split into longitudinal fibers (fibrillation)

Likely cause
Longitudinal stretching at 1:5–1:7 aligns the crystals along one axis and weakens transverse bonds; excessive stretching, a high calcite ratio or high oven/roll speed starts the splitting.
Solution
Anti-Split masterbatch builds strong bonds in the transverse direction; at 2.0–3.0%, break stoppages on the loom decrease by 40–60%.
Related product
Anti-Split Masterbatch
Durability

Raffia tape splits and breaks as the calcite ratio rises

Likely cause
Hard calcite particles cannot stretch during orientation, so micro-voids form around them; as the ratio rises, these voids merge.
Solution
Anti-Split masterbatch dampens the stress around calcite particles; on a sack line with 20–25% calcite, 2.0–3.0% raises bag drop and breaking strength.
Related product
Anti-Split Masterbatch
Odor & Gas

Products made from recycled (rPCR) raw material have a bad plastic odor

Likely cause
Recycled polymers have been in contact with food, detergent and oil residues, and degradation products are released during repeated thermal processing.
Solution
Odor-absorbing masterbatch traps VOC and aldehyde/amine-based molecules through chemical neutralization; 1.5% eliminates the plastic odor that develops in closed warehouses and hot environments.
Related product
Odor Eliminating Masterbatch
Odor & Gas

A strong odor is noticed when closed packaging is opened

Likely cause
Volatile odor molecules cannot escape and accumulate inside the pack.
Solution
Odor eliminating masterbatch binds these molecules within the material, so freshness is preserved even in a closed environment.
Related product
Odor Eliminating Masterbatch
Odor & Gas

Gas from the melt causes pores and voids in the product

Likely cause
Water vapor and volatile gases are released in the polymer melt at high temperature.
Solution
The active calcium oxide in antigas masterbatch chemically binds moisture and eliminates the gas source.
Related product
Desiccant & Antigas Masterbatch
Electrical

Products on the shelf attract dust and black dirt

Likely cause
Polyolefins have a very high surface resistance (>10¹⁵ Ω); friction builds static charge that attracts dust from the air.
Solution
Antistatic masterbatch lowers surface resistance to the 10⁹–10¹¹ Ω band; 1.5% stops static dust and black dirt pick-up.
Related product
Antistatic Masterbatch
Electrical

Operators get electric shocks on film winding lines, with a risk of sparks

Likely cause
Charge is transferred when surfaces rub or touch and separate (triboelectric effect); in insulating plastic this charge cannot dissipate and builds up.
Solution
Antistatic masterbatch increases surface conductivity for controlled discharge; on high-speed PP/PE film winding lines it eliminates operator shocks and the risk of sparks.
Related product
Antistatic Masterbatch
Electrical

The antistatic effect cannot be measured right after production

Likely cause
Internal antistatic agents need time to migrate to the surface and form the moisture-holding layer.
Solution
Test performance once it has stabilized; the waiting time depends on the polymer, thickness and temperature.
Related product
Antistatic Masterbatch

No matching problem found.

This table is compiled from the technical content on our site; for a definitive solution, consult our laboratory with your line conditions.

Related Pages

Let's find the right solution for your project

Contact our team for sample requests, color matching or technical consultancy.