Properties Relevant to Coloring and Additives
PA6 is a semi-crystalline polymer. Its melting temperature (Tm) is 215–225 °C, its glass transition temperature (Tg) is 50 °C and its density is 1.13–1.15 g/cm³. PA66 has a higher melting temperature, about 260 °C, than PA6 (about 220 °C). Typical melt temperature is 230–290 °C for PA6 and 270–300 °C for PA66; mold temperature is 40–90 °C for both.
- Moisture: Polyamide absorbs moisture and is prone to hydrolysis; drying before processing is critical.
- Thermal sensitivity: Because of the high processing temperature, antioxidant systems specific to PA are required; standard systems designed for polyolefins may not be sufficient.
- Migration: Migration risk is low in engineering plastics such as PA, PC and PET; grade 4–5 on the gray scale.
Recommended Colorex Masterbatches and Additives
- Mono masterbatch: Single pigment concentrates with a PA carrier are produced with a pigment loading of generally 25–50% for organic and 50–75% for inorganic pigments, and are generally used at 0.2–3.0%.
- Color masterbatch: Dedicated color series for polyamide are prepared after carrier compatibility is verified in the laboratory.
- Antioxidant masterbatch: Limits thermal degradation and yellowing with special antioxidant systems suited to polyamide's thermal sensitivity.
- Impact modifier and compatibilizer: MAH-grafted elastomer impact modifiers reduce the brittleness of PA6 and PA66 in the dry state; in glass-fiber PA, the compatibilizer strengthens the bond between fiber and matrix. 2.0–8.0% for impact improvement and 1.0–5.0% for MAH-grafted compatibilizer.
- Laser marking masterbatch: Used for permanent part and lot traceability in PA6/PA66 connectors, fuse boxes and sensor housings.
- Desiccant masterbatch: Complements pre-drying by binding free water remaining in the melt; it does not replace drying.
- Mold release masterbatch: The high-temperature series is made with components that run on PA lines without smoke or mold deposits; it eases demolding of glass-fiber parts.
Notes by Process
- Injection (technical parts): Mold temperature is in the 40–90 °C range for both types. In glass-fiber PA, mold release and compatibilizer additives reduce fiber marks on the surface and fiber pull-out from the matrix.
- Fiber and yarn (PA6): Pigment particles must be dispersed below 1 μm and the FPV must be below 1.0 bar/g. Against yellowing caused by thermal degradation and oxidation, a PA-compatible masterbatch with antioxidant should be used and the process temperature kept below 290 °C.
- Cable extrusion: Polyamide that has absorbed moisture foams when it leaves the die; for cable applications, drying the material in a vacuum oven at 80 °C for 4–6 hours before production is recommended.
Points to Watch
- Pigment heat resistance should be selected according to the PA type. Since PA66 melt temperature reaches 270–300 °C, pigments with a heat resistance above 300 °C, such as titanium dioxide, carbon black and iron oxide red, or phthalocyanine and DPP class pigments with 280–300 °C resistance, are preferred; diarylide yellow and orange (200–230 °C) and ultramarine blue (230–260 °C) are insufficient for these temperatures.
- The masterbatch and base polymer should be dried before processing; a desiccant additive only complements drying.
- A polymer-specific carrier should be used; an incompatible carrier causes phase separation and loss of mechanical properties.
Frequently Asked Questions
Is there a difference in masterbatch selection for PA6 and PA66?
Yes. PA66 has a higher melting temperature, about 260 °C, than PA6 (about 220 °C), and its typical melt temperature reaches 270–300 °C. For this reason, the pigments and carrier used in PA66 must have higher heat resistance.
Does desiccant masterbatch replace drying in polyamide?
No. Polyamide is highly moisture-sensitive and prone to hydrolysis. Desiccant masterbatch helps by binding free water remaining in the melt, but proper pre-drying is still required.
How can the brittleness of freshly molded PA parts be reduced?
Polyamide parts are brittle before moisture conditioning. MAH-grafted elastomer impact modifiers designed for engineering plastics increase the impact strength of PA6 and PA66 in the dry state and at low temperatures.